Some comments
Our niche was building 18 to 24 foot by 8 foot beam aluminum jet boats but have built up to 36 feet.
1) If you are not an extremely experienced ALUMINUM fabricator, don't try to heat the pieces to bend them. Just a slight hesitation when
applying the torch/heat and you will find the aluminum will just drop out of shape. This is considerably different than heating steel to a red hot phase and having it hold its shape. Aluminum oxide has a higher melting temperature than the aluminum underneath so the shape can be retained
until the outer temp is reached and entire section can just fall away. As an experiment, take a length of aluminum and heat it and you will discover what I am explaining. As we fit 1/4 inch stringers onto 1/4 inch hull bottoms, the welding heat from the welds would always introduce a bit of camber and we would heat the stringers to straighten them out. We had temp sticks, a crayon, that as we heated the stringer, we would just take the crayon and make a mark with it on the heated aluminum, if the crayon melted and got shiny, then that is the temp of the material. I do not want to give you inaccurate information here but, memory is questionable, I think we used 800 degree temp
2) The sweep of the bow appears quite tight. Generally if the bow has a fast or tight curve then the chine cannot also have the same tight turn or
the plate will not fit flat. As you have a plan from a known builder, there is a good chance that the two are compatible to make a developable surface
and that the sheet will in fact lie on both edges tightly.
As we built on a steel, male jig, we had tabs welded on the male jig and if a piece of aluminum was not snugging up, we would get under the jig and
drill up through the hull, drop a bolt in it and pull the plate down to the jig. After, just don't forget to weld up the holes.
3) I see that you have pieces of maybe plywood to make perhaps make a pattern for the sheet. You should make the template as one compete
piece, joining the ply with a thin batten at the 8 foot intervals, thin so that the shape or curve of your pattern is not impacted from the hard
spot that a heavy batten can produce at the joint. As this is a problem, on the 36 that we built, on a jig that was not proven to be developable, we took thin plywood, maybe 1/8 inch, cheap wall panelling, and made up a flat sheet about 40 feet by 4 feet wide by offsetting the sheets
and gluing them one on top of the other, so that the joints offset would act as a single piece.
If you make a template from small independent pieces there is a chance that you will have fitment issues.
4)I expect that your 20 foot sheets are long enough to make the side panels of the hull. If not, make the butt joint on a flat surface before
trying to weld it onto the framing/jig. Other wise you will have a disjointed joint, had to. You need the sheet to act as a single unit as when you bend it around a form to get a fair curve
5) We used 1/4 bottoms and 1/8 sides. I cannot see any reason why you would consider 1/4 for the sides. On the 36, we used a 3/16 side but then
it was 36 feet long.
6) Welding. Unless absolutely critical, I would not use Tig on a boat hull. The slow speed of tig 7) welding introduces a lot of aluminum expansion
into the sheet so that you actually can weld in deformation in the hull. Some will say not, and occasionally we used Tig but not often.
When you are doing a butt weld you must cut out the backside of the weld before welding the backside. Most important!!
7) When welding in any other structure, to the hull or most anywhere else, try to ensure that you have a weld bead on each side of each other.
Aluminum work hardens extremely easy. If you weld say a 1/4 inch piece onto another 1/4 inch piece only on one side, it is extremely easy
to break this weld due to stress concentration. And the stress concentration due to the notch effect can cause failure due to small localized work hardening
8) Also when you start and stop any long seams, you must cut back the bead where you stopped to ensure that when you stopped the first bead
there was not a weld crevice due to the bead cooling quickly. You can try this out on some scrap. If you get to the end of the weld, just
draw back the wirefeed to minimize this effect, but we always cut the end of the weld bead back say 1/2 inch to ensure a fresh start of the next continuous bead
9) When butt welding sheets, the weld must be cut from the back side to welded material. We used a standard 7 1/4 inch skil saw, and would cut
the weld from the backside down until the thin black line of the unwelded plate disappeared.
If I think of anything else I will let you know